Sahar A. Fadlallah, Mohammed A. Amin, Ghaida S. Alosaimi. Construction of Nanophase Novel Coatings-Based Titanium for the Enhancement of Protein Adsorption[J]. Acta Metallurgica Sinica (English Letters), 2016, 29(3): 243-252.
Fig. 1 SEM/EDX examinations of polished Ti a, TNP after Ti etched in lactic acid/NH4F bath for 4 h b, ATNP surface after anodization of TNP for 2 h in 0.5 mol/L HCl/glycerol at 20 V c, Ag-ATNP surface after soaking ATNP in 0.1 mol/L AgNO3 for 30 min d, Au-ATNP surface after soaking in HAuCl3 for 30 min e
| Sample | Ti | O | C | Cl | Ag | Au | N | Na |
|---|---|---|---|---|---|---|---|---|
| Ti | 100 | - | - | - | - | - | - | - |
| TNP | 97.12 | - | - | - | - | - | 2.88 | - |
| ATNP | 84.28 | 15.72 | - | - | - | - | - | - |
| Ag-ATNP | 77.10 | 17.40 | - | - | 1.60 | - | - | - |
| Au-ATNP | 80.85 | 17.72 | - | - | - | 1.72 | - | - |
Table 1 Chemical composition of Ti, TNP, ATNP, Ag-ATNP and Au-ATNP samples before immersion, based on ZAF software (in wt%)
| Sample | Ti | O | C | Cl | Ag | Au | N | Na |
|---|---|---|---|---|---|---|---|---|
| Ti | 100 | - | - | - | - | - | - | - |
| TNP | 97.12 | - | - | - | - | - | 2.88 | - |
| ATNP | 84.28 | 15.72 | - | - | - | - | - | - |
| Ag-ATNP | 77.10 | 17.40 | - | - | 1.60 | - | - | - |
| Au-ATNP | 80.85 | 17.72 | - | - | - | 1.72 | - | - |
| Sample | Ti | O | C | Cl | Ag | Au | N | Na |
|---|---|---|---|---|---|---|---|---|
| Ti | 75.47 | - | 10.54 | 2.52 | - | - | 7.40 | 4.44 |
| TNP | 88.95 | - | - | - | - | - | 11.05 | - |
| ATNP | 90.72 | - | - | - | - | - | 9.28 | - |
| Ag-ATNP | 90.59 | - | - | - | - | - | 9.41 | - |
| Au-ATNP | 89.88 | - | - | - | - | - | 10.12 | - |
Table 2 Chemical composition of Ti, TNP, ATNP, Ag-ATNP and Au-ATNP samples after immersion in HBSS solution containing 2.9 g/L BSA for 7 days at 37 °C, based on ZAF software (in wt%)
| Sample | Ti | O | C | Cl | Ag | Au | N | Na |
|---|---|---|---|---|---|---|---|---|
| Ti | 75.47 | - | 10.54 | 2.52 | - | - | 7.40 | 4.44 |
| TNP | 88.95 | - | - | - | - | - | 11.05 | - |
| ATNP | 90.72 | - | - | - | - | - | 9.28 | - |
| Ag-ATNP | 90.59 | - | - | - | - | - | 9.41 | - |
| Au-ATNP | 89.88 | - | - | - | - | - | 10.12 | - |
Fig. 2 EIS spectra for TNP, ATNP, Ag-ATNP and Au-ATNP samples after 7 days of immersion in HBSS at 37 °C, comparing with Ti: a Nyquist plots; b Bode plots; c equivalent circuit (R s(R p Q p)(R b Q b))
| Implant surface | BSA concentration (g/L) | R s(Ω) | Q p | R p(kΩ cm2) | n p | C p(µF/cm2) | Q b | R b(kΩ cm2) | n b | C b(µF/cm2) | R ct(kΩ cm2) | θ(°) | χ 2 |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Ti | 0 | 10.8 | 18.6 | 631 | 0.89 | 25.24 | 577.4 | 15 | 0.78 | 1061.6 | 646 | 77.8 | 0.1 |
| 0.2 | 14.9 | 15.81 | 980 | 0.99 | 16.25 | 797.6 | 16 | 0.92 | 995.2 | 996 | 81.8 | 0.4 | |
| 2.9 | 18 | 15.14 | 989 | 0.98 | 16.1 | 929.7 | 11 | 0.84 | 1447.6 | 1000 | 78.9 | 0.2 | |
| 6 | 19.1 | 13.31 | 986 | 0.93 | 16.15 | 255.1 | 17 | 0.53 | 936.7 | 1003 | 81.7 | 0.04 | |
| TNP | 0 | 10 | 19.86 | 780 | 0.99 | 20.42 | 572.2 | 16 | 0.8 | 995.2 | 796 | 78 | 0.08 |
| 0.2 | 10.3 | 11.9 | 984 | 0.89 | 16.18 | 653.6 | 17 | 0.87 | 936.7 | 1001 | 80.2 | 0.9 | |
| 2.9 | 10.5 | 15.2 | 990 | 0.98 | 16.08 | 444.4 | 25 | 0.87 | 636.9 | 1015 | 81.6 | 0.9 | |
| 6 | 9.7 | 14.04 | 988 | 0.95 | 16.12 | 427.8 | 22 | 0.81 | 723.8 | 1010 | 82.6 | 0.9 | |
| ATNP | 0 | 24.4 | 3.87 | 4000 | 0.99 | 3.98 | 61.05 | 150 | 0.8 | 106.2 | 4150 | 85.8 | 0.6 |
| 0.2 | 68 | 2.89 | 4300 | 0.91 | 3.7 | 70.75 | 166 | 0.89 | 95.93 | 4466 | 84.6 | 0.9 | |
| 2.9 | 36 | 3 | 3600 | 0.86 | 4.42 | 28.95 | 172 | 0.58 | 92.6 | 3772 | 81.3 | 0.9 | |
| 6 | 41.5 | 2.21 | 7000 | 0.99 | 2.27 | 45.58 | 190 | 0.78 | 83.81 | 7190 | 80.2 | 0.02 | |
| Ag-ATNP | 0 | 35.4 | 2.52 | 5000 | 0.93 | 3.06 | 12.46 | 200 | 0.63 | 79.62 | 5200 | 83 | 0.05 |
| 0.2 | 33.7 | 3.11 | 4460 | 0.95 | 3.57 | 33.97 | 255 | 0.78 | 62.45 | 4715 | 83.1 | 0.9 | |
| 2.9 | 38.5 | 3.26 | 4500 | 0.97 | 3.54 | 39.33 | 260 | 0.84 | 61.24 | 4760 | 81.1 | 0.4 | |
| 6 | 29 | 2.2 | 4400 | 0.82 | 3.62 | 33.91 | 270 | 0.8 | 58.98 | 4670 | 83.9 | 0.9 | |
| Au-ATNP | 0 | 35 | 1.88 | 8000 | 0.98 | 1.99 | 39.42 | 149 | 0.64 | 106.7 | 8149 | 83.1 | 0.3 |
| 0.2 | 32.9 | 2.04 | 6600 | 0.94 | 2.41 | 37.25 | 220 | 0.76 | 72.38 | 6820 | 84.6 | 0.5 | |
| 2.9 | 31.7 | 1.85 | 7500 | 0.95 | 2.12 | 28.19 | 275 | 0.74 | 57.9 | 7775 | 81.3 | 0.8 | |
| 6 | 31.3 | 1.73 | 7800 | 0.94 | 2.04 | 41.94 | 280 | 0.89 | 56.87 | 8080 | 80.2 | 0.1 |
Table 3 EIS equivalent circuit (R s(R P Q p)(R b Q b)) parameters for Ti, TNP, ATNP, Ag-ATNP and Au-ATNP implants surfaces after 7 days of immersion in HBSS containing 0-6 g/L BSA at 37 °C
| Implant surface | BSA concentration (g/L) | R s(Ω) | Q p | R p(kΩ cm2) | n p | C p(µF/cm2) | Q b | R b(kΩ cm2) | n b | C b(µF/cm2) | R ct(kΩ cm2) | θ(°) | χ 2 |
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Ti | 0 | 10.8 | 18.6 | 631 | 0.89 | 25.24 | 577.4 | 15 | 0.78 | 1061.6 | 646 | 77.8 | 0.1 |
| 0.2 | 14.9 | 15.81 | 980 | 0.99 | 16.25 | 797.6 | 16 | 0.92 | 995.2 | 996 | 81.8 | 0.4 | |
| 2.9 | 18 | 15.14 | 989 | 0.98 | 16.1 | 929.7 | 11 | 0.84 | 1447.6 | 1000 | 78.9 | 0.2 | |
| 6 | 19.1 | 13.31 | 986 | 0.93 | 16.15 | 255.1 | 17 | 0.53 | 936.7 | 1003 | 81.7 | 0.04 | |
| TNP | 0 | 10 | 19.86 | 780 | 0.99 | 20.42 | 572.2 | 16 | 0.8 | 995.2 | 796 | 78 | 0.08 |
| 0.2 | 10.3 | 11.9 | 984 | 0.89 | 16.18 | 653.6 | 17 | 0.87 | 936.7 | 1001 | 80.2 | 0.9 | |
| 2.9 | 10.5 | 15.2 | 990 | 0.98 | 16.08 | 444.4 | 25 | 0.87 | 636.9 | 1015 | 81.6 | 0.9 | |
| 6 | 9.7 | 14.04 | 988 | 0.95 | 16.12 | 427.8 | 22 | 0.81 | 723.8 | 1010 | 82.6 | 0.9 | |
| ATNP | 0 | 24.4 | 3.87 | 4000 | 0.99 | 3.98 | 61.05 | 150 | 0.8 | 106.2 | 4150 | 85.8 | 0.6 |
| 0.2 | 68 | 2.89 | 4300 | 0.91 | 3.7 | 70.75 | 166 | 0.89 | 95.93 | 4466 | 84.6 | 0.9 | |
| 2.9 | 36 | 3 | 3600 | 0.86 | 4.42 | 28.95 | 172 | 0.58 | 92.6 | 3772 | 81.3 | 0.9 | |
| 6 | 41.5 | 2.21 | 7000 | 0.99 | 2.27 | 45.58 | 190 | 0.78 | 83.81 | 7190 | 80.2 | 0.02 | |
| Ag-ATNP | 0 | 35.4 | 2.52 | 5000 | 0.93 | 3.06 | 12.46 | 200 | 0.63 | 79.62 | 5200 | 83 | 0.05 |
| 0.2 | 33.7 | 3.11 | 4460 | 0.95 | 3.57 | 33.97 | 255 | 0.78 | 62.45 | 4715 | 83.1 | 0.9 | |
| 2.9 | 38.5 | 3.26 | 4500 | 0.97 | 3.54 | 39.33 | 260 | 0.84 | 61.24 | 4760 | 81.1 | 0.4 | |
| 6 | 29 | 2.2 | 4400 | 0.82 | 3.62 | 33.91 | 270 | 0.8 | 58.98 | 4670 | 83.9 | 0.9 | |
| Au-ATNP | 0 | 35 | 1.88 | 8000 | 0.98 | 1.99 | 39.42 | 149 | 0.64 | 106.7 | 8149 | 83.1 | 0.3 |
| 0.2 | 32.9 | 2.04 | 6600 | 0.94 | 2.41 | 37.25 | 220 | 0.76 | 72.38 | 6820 | 84.6 | 0.5 | |
| 2.9 | 31.7 | 1.85 | 7500 | 0.95 | 2.12 | 28.19 | 275 | 0.74 | 57.9 | 7775 | 81.3 | 0.8 | |
| 6 | 31.3 | 1.73 | 7800 | 0.94 | 2.04 | 41.94 | 280 | 0.89 | 56.87 | 8080 | 80.2 | 0.1 |
Fig. 3 EIS spectra for Ti a, TNP b, ATNP c, Ag-ATNP d, Au-ATNP e after 7 days of immersion in HBSS containing various BSA concentrations ranging from 0 to 6 g/L at 37 °C as Nyquist plots with inserted bode phase plots
Fig. 4 SEM/EDX examinations of Ti a, TNP b, ATNP c, Ag-ATNP d, Au-ATNP e surface topography after 7 days of immersion in HBSS containing 2.9 g/L BSA at 37 °C
Fig. 5 Langmuir adsorption isotherm presented in a linear form for BSA adsorbed onto Ti a, TNP b, ATNP c, Ag-ATNP d, Au-ATNP e in HBSS containing various concentration of BSA ranging from 0 to 6 g/L solution at 37 °C
| [1] | W.Q. Yu, Y.L. Zhang, X.Q. Jiang, F.Q. Zhang, Oral Dis. 16, 624(2010) |
| [2] | C.C. Mohan, K.P. Chennazhi, D. Menon, Acta Biomater. 9, 9568(2013) |
| [3] | W.Q. Yu, J. Qiu, F.Q. Zhang, Colloids Surf. B 84, 400 (2011) |
| [4] | A. Wennerberg, T. Albrektsson, C. Johansson, B. Andersson, Biomaterials 17, 15 (1996) |
| [5] | H.W. Kim, Y.H. Koh, L.H. Li, S. Lee, H.E. Kim, Biomaterials 25, 2533 (2004) |
| [6] | S. Nishiguchi, H. Kato, H. Fujita, M. Oka, H.M. Kim, T. Kokubo, T. Nakamura, Biomaterials 22, 2525 (2001) |
| [7] | H.J. Song, S.H. Park, S.H. Jeong, Y.J. Park, J. Mater. Process. Technol. 209, 864(2009) |
| [8] | J.I. Lim, B. Yu, K.M. Woo, Y.K. Lee, Appl. Surf. Sci. 255, 2456(2008) |
| [9] | A. Al-Ahmad, M.W. Al-Ahmad, A. Fackler, M. Follo, E. Hellwig, M. Bächle, C. Hannig, J.S. Han, M. Wolkewitz, R. Kohal, Arch. Oral Biol. 58, 1139(2013) |
| [10] | J.J. Ryu, S. Letchuman, P. Shrotriya, J. Mech. Behav. Biomed. Mater. 14(5), 55(2012) |
| [11] | F. Rupp, R.A. Gittens, L. Scheideler, A. Marmur, B.D. Boyan, Z. Schwartz, J.G. Gerstorfer, Acta Biomater. 10, 2894(2014) |
| [12] | S. Wu, X. Liu, W.K. Yeung, H. Guo, P. Li, T. Hu, C.Y. Chung, P.K. Chu, Surf. Coat. Technol. 233, 13(2013) |
| [13] | N. Wang, H. Li, W. Lü, J. Li, J. Wang, Z. Zhang, Y. Liu, Biomaterials 32, 6900 (2011) |
| [14] | Y. Shibata, Y. Tanimoto, J. Prosthodont. Res. 59, 20(2015) |
| [15] | Y. Tian, H. Cao, Y. Qiao, F. Meng, X. Liu, Acta Biomater. 10, 4505(2014) |
| [16] | H. Wu, X. Zhang, X. He, M. Li, X. Huang, R. Hang, B. Tang, Appl. Surf. Sci. 317, 614(2014) |
| [17] | H. Li, Q. Cui, B. Feng, J. Wang, X. Lu, J. Weng, Appl. Surf. Sci. 284, 179(2013) |
| [18] | G. Mani, D.M. Johnson, D. Marton, M.D. Feldman, D. Patel, A.A. Ayon, C. Mauli Agrawal, Biomaterials 29, 4561(2008) |
| [19] | S.M.F. Gad El-Rab, S.A. Fadl-allah, A.A. Montser, Appl. Surf. Sci. 261, 1(2012) |
| [20] | J.A. Lyndon, B.J. Boyd, N. Birbilis, J. Control. Release 179, 63 (2014) |
| [21] | S.B. Goodman, Z. Yao, M. Keeney, F. Yang, Biomaterials 34, 3174 (2013) |
| [22] | M.M. Speeckaert, R. Speeckaert, N.V. Geel, J.R. Delanghe, Adv. Clin. Chem. 63, 1(2014) |
| [23] | K. Mark, J. Park, Mater. Sci. 58, 327(2013) |
| [24] | J.Y. Lim, M.C. Shaughnessy, Z. Zhou, H. Noh, E.A. Vogler, H.J. Donahue, Biomaterials 29, 1778 (2008) |
| [25] | S. Sista, C. Wen, P.D. Hodgson, G. Pande, Mater. Sci. Eng. C 33, 1573 (2013) |
| [26] | P. Silva-Bermudez, S.E. Rodil, Surf. Coat. Technol. 233, 147(2013) |
| [27] | W.A. Badawy, A.M. Fathi, R.M. El-Sherief, S.A. Fadl-Allah, J. Alloys Compd. 475, 911(2009) |
| [28] | S.A. Fadl-allah, Q. Mohsen, Appl. Surf. Sci. 256, 5849(2010) |
| [29] | C. Matschegewski, S. Staehlke, R. Loeffler, R. Lange, F. Chai, D.P. Kern, U. Beck, B.J. Nebe, Biomaterials 31, 5729 (2012) |
| [30] | N.S. El-Shenawy, Q. Mohsen, S.A. Fadl-allah, J. Mater. Sci. Mater. Med. 23, 1763(2012) |
| [31] | N.I.Z. Abidin, A.D. Atrens, D. Martin, A. Atrens, Corros. Sci. 53, 3542(2011) |
| [32] | Q. Zhao, T. Cao, Mater. Sci. Eng. B 172, 163 (2010) |
| [33] | F.M.B. Hassan, H. Nanjo, S. Venkatachalam, M. Kanakubo, T. Ebina, Electrochim. Acta 55, 3130 (2010) |
| [34] | C.F. Almeida Alves, F. Oliveira, I. Carvalho, A.P. Piedade, S. Carvalho, Mater. Sci. Eng. C 34, 22 (2014) |
| [35] | Y. Zhang, R. Yuan, Y. Chai, Y. Xiang, X. Qian, H. Zhang, J. Colloid Interface Sci. 341, 108(2010) |
| [36] | P.D.V. ConCellos, S. Bose, H. Beyenal, A. Bandyopadhyay, L.G. Zirkle, Mater. Sci. Eng. C 32, 1112 (2012) |
| [37] | S. Eraković, A. Janković, C. Ristoscu, L. Duta, N. Serban, A. Visan, I.N. Mihailescu, G.E. Stan, M. Socol, O. Iordache, I. Dumitrescu, C.R. Luculescu, D.J. Janaćković, V.M. Stanković, Appl. Surf. Sci. 293, 37(2014) |
| [38] | U. Rammelt, N. Hebestreit, A. Fikus, W. Plieth, Electrochim. Acta 46, 2363 (2001) |
| [39] | L. Zhao, H. Wang, K. Huo, L. Cui, W. Zhang, H. Ni, Y. Zhang, Z. Wu, P.K. Chu, Biomaterials 32, 5706 (2011) |
| [40] | R.K. Mohanty, S. Thennarasu, A.B. Mandal, Colloids Surf. B 114, 138 (2014) |
| [41] | H. Cai, P. Yao, Colloids Surf. B 123, 900 (2014) |
| [42] | W. Wang, F. Mohammadi, A. Alfantazi, Corros. Sci. 57, 11(2012) |
| [43] | D. Kowalski, D. Kim, P. Schmuki, Nano Today 8, 235 (2013) |
| [44] | S. Karimi, T. Nickchi, A. Alfantazi, Corros. Sci. 53, 3262(2011) |
| [45] | D.C. Hansen, G.W. Luther, J.H. Waite, J. Colloid Interface Sci. 168, 206(1994) |
| [46] | Z. Rong, Y. Zhao, B. Liu, Y. Tian, B. Yang, J. Electroanal. Chem. 707, 102(2013) |
| [47] | J. Zhang, A.M. Bond, J. Electroanal. Chem. 574, 299(2005) |
| [1] | Peng Han, Wen Wang, Jun Cai, Jia Lin, Hubin Yang, Qianzhi Ma, Feng Gao, Ke Qiao, Fengming Qiang, Kuaishe Wang. Excellent superplasticity for lamellar microstructure in nugget of a double-sided friction stir welded Ti-4.5Al-3V-2Mo-2Fe alloy joint [J]. Metals Advances, 2026, 40(2): 110-123. |
| [2] | Zhizhi Wang, Pei Liu, Jingyi Guo, Yiwen Yan, Aiqin Wang, Jingpei Xie. Excellent mechanical properties and biocompatibility of Ti-15Mo alloy via interstitial nitrogen atoms [J]. Metals Advances, 2026, 39(1): 38-46. |
| [3] | Author links open overlay panelXiaodong Yang, Chang Liu, Lechun Xie. Surface engineering of medical titanium alloy: A review [J]. Metals Advances, 2026, 39(1): 95-116. |
| [4] | H. Q. Dai, N. Li, L. H. Wu, J. Wang, P. Xue, F. C. Liu, D. R. Ni, B. L. Xiao, Z. Y. Ma. Low-Temperature Superplastic Deformation Behavior of Bimodal Microstructure of Friction Stir Processed Ti-6Al-4V Alloy [J]. Acta Metallurgica Sinica (English Letters), 2025, 38(9): 1559-1569. |
| [5] | Yunlu Jiang, Lihui Wu, Dingrui Ni, Hongbo Zhao, Xu Han, Peng Xue, Bolv Xiao, Zongyi Ma. Effect of Post Weld Heat Treatment on Residual Stress and Mechanical Properties of 106 mm Thick TC4 Titanium Alloy Electron Beam Welded Joints [J]. Acta Metallurgica Sinica (English Letters), 2025, 38(7): 1083-1094. |
| [6] | Xu Yue, Zhiyong Chen, Wei Chen, Qingjiang Wang. Hot Deformation Behavior and Processing Map of a Novel Ti750s High-Temperature Titanium Alloy [J]. Acta Metallurgica Sinica (English Letters), 2025, 38(7): 1174-1194. |
| [7] | Wangjian Yu, Rui Hu, Guoqiang Shang, Xian Luo, Hong Wang. Correlation Mechanism Between Microstructure and Fatigue Crack Propagation Behavior of Ti-Mo-Cr-V-Nb-Al Titanium Alloys [J]. Acta Metallurgica Sinica (English Letters), 2025, 38(6): 981-1002. |
| [8] | X. W. Shang, Z. G. Lu, R. P. Guo, L. Xu. Influence of Hot Isostatic Pressing Temperature on Microstructure and Mechanical Properties of Ti-6.5Al-3.5Mo-1.5Zr-0.3Si Alloy [J]. Acta Metallurgica Sinica (English Letters), 2025, 38(4): 627-641. |
| [9] | Yiyun Guo, Lei Wu, Yibo Shang, Chengqi Sun. Effects of Defect, Mean Stress and Lower Loading on High Cycle and Very High Cycle Fatigue Behavior of Ti-6Al-4V Alloy [J]. Acta Metallurgica Sinica (English Letters), 2025, 38(3): 435-448. |
| [10] | Cheng Ren, Xiaohua Min, Sujie Zhang, Weiqiang Wang. Springback Behavior and Biocompatibility in β-Type Ti-Mo-O Alloys [J]. Acta Metallurgica Sinica (English Letters), 2025, 38(2): 313-326. |
| [11] | Qi-Mei Tian, Fu Xiao, Ya Yang, Yuan-Biao Tan, Song Xiang, Xuan-Ming Ji, Fei Zhao, Hui Yang. Achieving an Extraordinary Strength-Ductility Synchronization in TA15 Titanium Alloy via Tailoring a Tri-modal Microstructure [J]. Acta Metallurgica Sinica (English Letters), 2025, 38(12): 2228-2242. |
| [12] | Xiangru Guo, Jian Zhang, Tieqiang Kong, Junjie Shen, Qingjian Liu, Chaoyang Sun, Peipei Li. Unraveling the Discontinuous Dynamic Recrystallization of the TC17 Titanium Alloy during Hot Deformation by Crystal Plasticity Modeling [J]. Acta Metallurgica Sinica (English Letters), 2025, 38(12): 2243-2264. |
| [13] | Junchen Fan, Ruidong Liu, Xiaofang Wang. Nitridation of Magnesium and its Application in Corrosion Resistance: A Review [J]. Acta Metallurgica Sinica (English Letters), 2025, 38(11): 1873-1890. |
| [14] | Xinrui Gu, Xudong Yuan, Tingyi Yan, Biao Li, Haojie Liang, Jingyu Pang, Huameng Fu, Hongwei Zhang, Long Zhang. Microstructural Evolution and Mechanical Properties of Graphene Nanoplatelet Reinforced Ti-6Al-4V Matrix Composites [J]. Acta Metallurgica Sinica (English Letters), 2025, 38(11): 1991-2000. |
| [15] | Yuan Jiang, Baizhi Liang, Shewei Xin, Lei Shi, Siyuan Zhang, Kai Zhang, Hao Wang, Yi Yang, Lai-Chang Zhang. Cyclic Heat Treatment Induced Spheroidization of α Phase in Ti-5Al-3Mo-3V-2Cr-2Zr-1Nb-1Fe Alloy [J]. Acta Metallurgica Sinica (English Letters), 2025, 38(10): 1827-1838. |
| Viewed | ||||||
|
Full text |
|
|||||
|
Abstract |
|
|||||
WeChat