Acta Metallurgica Sinica (English Letters) ›› 2019, Vol. 32 ›› Issue (2): 145-168.DOI: 10.1007/s40195-018-00871-2
• Orginal Article • Next Articles
Shuai-Ju Meng1, Hui Yu1(
), Shao-Da Fan1, Qi-Zhi Li1, Sung Hyuk Park2, Joung Sik Suh3, Young Min Kim3, Xiao-Long Nan4, Ming-Zhe Bian5, Fu-Xing Yin1, Wei-Min Zhao1, Bong Sun You3, Kwang Seon Shin6
Received:2018-11-04
Revised:2018-12-04
Online:2019-01-17
Published:2019-02-13
Shuai-Ju Meng, Hui Yu, Shao-Da Fan, Qi-Zhi Li, Sung Hyuk Park, Joung Sik Suh, Young Min Kim, Xiao-Long Nan, Ming-Zhe Bian, Fu-Xing Yin, Wei-Min Zhao, Bong Sun You, Kwang Seon Shin. Recent Progress and Development in Extrusion of Rare Earth Free Mg Alloys: A Review[J]. Acta Metallurgica Sinica (English Letters), 2019, 32(2): 145-168.
Add to citation manager EndNote|Ris|BibTeX
| Compositions (wt%) | Extrusion parameters T, v (m/min), r | TYS (MPa) | UTS (MPa) | EL (%) | YR | Ref. |
|---|---|---|---|---|---|---|
| AZ80-0.5Ca | 450°C, -, 12:1, T5 | 180 | 253 | 7.8 | - | [ |
| Mg-4Al-2Sr-0.3Mn | 360°C, -, - | 262.4 | 296.4 | 6.2 | - | [ |
| Mg-4Al-2Sr-1Ca-0.3Mn | 360°C, -, - | 299.1 | 326.7 | 3.6 | - | |
| AM80 | 250°C, 15.06, 25:1 | 178 | 319 | 17.1 | - | [ |
| AM80-3Sn | 250°C, 15.06, 25:1 | 199 | 340 | 16 | - | |
| AM80-5Sn | 250°C, 15.06, 25:1 | 242 | 349 | 9.9 | - | |
| AM80-7Sn | 250°C, 15.06, 25:1 | 251 | 345 | 8.2 | - | |
| ATM110 | 300°C, 25, 25:1 | 260 | 292 | 21.0 | 0.89 | [ |
| ATM310 | 250°C, 25, 25:1 | 229 | 293 | 16.0 | 0.88 | |
| 300°C, 25, 25:1 | 213 | 281 | 20.5 | 0.76 | ||
| 350°C, 25, 25:1 | 201 | 271 | 20.0 | 0.74 | ||
| ATM610 | 250°C, 25, 25:1 | 241 | 319 | 12.0 | 0.76 | |
| ATM130 | 300°C, 25, 25:1 | 253 | 288 | 19.5 | 0.85 | |
| ATM330 | 250°C, 25, 25:1 | 225 | 306 | 15.4 | 0.74 | |
| ATM630 | 250°C, 25, 25:1 | 220 | 318 | 8.6 | 0.69 | |
| Mg-8Al-4Sn-2Zn-0.15Mn | 250°C, 0.12, 20:1 | 371 | 415 | 9.1 | 1.02 | [ |
| AZ82 | 250°C, 1.2, 20:1 | 233 | 347 | 13.4 | 0.97 | [ |
| AZT822 | 250°C, 1.2, 20:1 | 258 | 361 | 11.2 | 1.03 | |
| AZT824 | 250°C, 1.2, 20:1 | 280 | 370 | 10.1 | 1.09 | |
| AZT826 | 250°C, 1.2, 20:1 | 287 | 354 | 7.8 | 1.09 | |
| Mg-3.6Al-3.3Ca-0.4Mn | DC, 350°C, 0.12, 20:1 | 410 | 420 | 5.6 | 0.83 | [ |
| Mg-3.6Al-3.3Ca-0.4Mn | PM, 350°C, 0.12, 20:1 | 304 | 314 | 9.5 | 0.81 | [ |
| Mg-3.6Al-3.3Ca-0.4Mn | DC, 400°C, 0.12, 20:1 | 409 | 413 | 8 | 0.82 | |
| Mg-0.30Al-0.21Ca-0.47Mn | 350°C, 60, 20:1 | 206 | 240 | 29 | 0.68 | [ |
| 400°C, 60, 20:1 | 200 | 233 | 24 | 0.65 | ||
| 450°C, 60, 20:1 | 190 | 233 | 20 | 0.55 | ||
| 500°C, 60, 20:1 | 177 | 222 | 17.5 | 0.54 | ||
| Mg-0.30Al-0.21Ca-0.47Mn | 500°C, 60, 20:1, T5 | 207 | 254 | 13.6 | - | [ |
| Mg-0.30Al-0.21Ca-0.47Mn | 500°C, 60, 20:1 | 170 | 218 | 15.5 | - | |
| AZ31 | 500°C, 1.2, 20:1, T5 | 177 | 248 | 20 | - | |
| Mg-0.31Al-0.19Ca-0.43Mn | 275°C, 24, 20:1, T6 | 230 | 262 | 26 | 0.72 | [ |
| Mg-1.19Al-0.20Ca-0.46Mn | 275°C, 24, 20:1, T6 | 287 | 306 | 20 | 0.67 | |
| Mg-2.48Al-0.20Ca-0.44Mn | 275°C, 24, 20:1, T6 | 240 | 283 | 18 | 0.62 |
Table 1 Typical mechanical properties of selected Mg-Al-based extrusion alloys [21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31]
| Compositions (wt%) | Extrusion parameters T, v (m/min), r | TYS (MPa) | UTS (MPa) | EL (%) | YR | Ref. |
|---|---|---|---|---|---|---|
| AZ80-0.5Ca | 450°C, -, 12:1, T5 | 180 | 253 | 7.8 | - | [ |
| Mg-4Al-2Sr-0.3Mn | 360°C, -, - | 262.4 | 296.4 | 6.2 | - | [ |
| Mg-4Al-2Sr-1Ca-0.3Mn | 360°C, -, - | 299.1 | 326.7 | 3.6 | - | |
| AM80 | 250°C, 15.06, 25:1 | 178 | 319 | 17.1 | - | [ |
| AM80-3Sn | 250°C, 15.06, 25:1 | 199 | 340 | 16 | - | |
| AM80-5Sn | 250°C, 15.06, 25:1 | 242 | 349 | 9.9 | - | |
| AM80-7Sn | 250°C, 15.06, 25:1 | 251 | 345 | 8.2 | - | |
| ATM110 | 300°C, 25, 25:1 | 260 | 292 | 21.0 | 0.89 | [ |
| ATM310 | 250°C, 25, 25:1 | 229 | 293 | 16.0 | 0.88 | |
| 300°C, 25, 25:1 | 213 | 281 | 20.5 | 0.76 | ||
| 350°C, 25, 25:1 | 201 | 271 | 20.0 | 0.74 | ||
| ATM610 | 250°C, 25, 25:1 | 241 | 319 | 12.0 | 0.76 | |
| ATM130 | 300°C, 25, 25:1 | 253 | 288 | 19.5 | 0.85 | |
| ATM330 | 250°C, 25, 25:1 | 225 | 306 | 15.4 | 0.74 | |
| ATM630 | 250°C, 25, 25:1 | 220 | 318 | 8.6 | 0.69 | |
| Mg-8Al-4Sn-2Zn-0.15Mn | 250°C, 0.12, 20:1 | 371 | 415 | 9.1 | 1.02 | [ |
| AZ82 | 250°C, 1.2, 20:1 | 233 | 347 | 13.4 | 0.97 | [ |
| AZT822 | 250°C, 1.2, 20:1 | 258 | 361 | 11.2 | 1.03 | |
| AZT824 | 250°C, 1.2, 20:1 | 280 | 370 | 10.1 | 1.09 | |
| AZT826 | 250°C, 1.2, 20:1 | 287 | 354 | 7.8 | 1.09 | |
| Mg-3.6Al-3.3Ca-0.4Mn | DC, 350°C, 0.12, 20:1 | 410 | 420 | 5.6 | 0.83 | [ |
| Mg-3.6Al-3.3Ca-0.4Mn | PM, 350°C, 0.12, 20:1 | 304 | 314 | 9.5 | 0.81 | [ |
| Mg-3.6Al-3.3Ca-0.4Mn | DC, 400°C, 0.12, 20:1 | 409 | 413 | 8 | 0.82 | |
| Mg-0.30Al-0.21Ca-0.47Mn | 350°C, 60, 20:1 | 206 | 240 | 29 | 0.68 | [ |
| 400°C, 60, 20:1 | 200 | 233 | 24 | 0.65 | ||
| 450°C, 60, 20:1 | 190 | 233 | 20 | 0.55 | ||
| 500°C, 60, 20:1 | 177 | 222 | 17.5 | 0.54 | ||
| Mg-0.30Al-0.21Ca-0.47Mn | 500°C, 60, 20:1, T5 | 207 | 254 | 13.6 | - | [ |
| Mg-0.30Al-0.21Ca-0.47Mn | 500°C, 60, 20:1 | 170 | 218 | 15.5 | - | |
| AZ31 | 500°C, 1.2, 20:1, T5 | 177 | 248 | 20 | - | |
| Mg-0.31Al-0.19Ca-0.43Mn | 275°C, 24, 20:1, T6 | 230 | 262 | 26 | 0.72 | [ |
| Mg-1.19Al-0.20Ca-0.46Mn | 275°C, 24, 20:1, T6 | 287 | 306 | 20 | 0.67 | |
| Mg-2.48Al-0.20Ca-0.44Mn | 275°C, 24, 20:1, T6 | 240 | 283 | 18 | 0.62 |
Fig. 1 a, b TEM images of as-extruded Mg-3.6Al-3.3Ca-0.4Mn (wt%) sample, c high-angle annular dark field image of the unDRXed area, d 3DAP elemental mapping of Al, Ca and Mn for the precipitates in as-extruded sample. Each dot represents one atom [28]
| Compositions (wt%) | Extrusion parameters T, v (m/min), r | YS (MPa) | UTS (MPa) | El (%) | YR | Ref. |
|---|---|---|---|---|---|---|
| Mg-1.0Zn | 350°C, 0.12, 16:1 | 148 | 230 | 16.2 | - | [ |
| Mg-2Zn | 320°C, -, 23.6:1 | 115 | 192 | 22.8 | - | [ |
| Mg-6Zn | 250°C, -, 8:1 | 169.5 | 279.5 | 18.8 | - | [ |
| Mg-6.2Zn (Z6) | 350°C, 0.12, 20:1. | 162 | 290 | 21 | - | [ |
| 350°C, 0.12, 20:1, T6 | 254 | 318 | 17.3 | - | ||
| Mg-6.2Zn-0.6Zr | 350°C, 0.12, 20:1. | 244 | 317 | 13.8 | - | |
| 350°C, 0.12, 20:1, T6 | 275 | 318 | 17.1 | - | ||
| Mg-6Zn-0.2Ca | 300°C, 0.12, 20:1 | 148 | 275 | 26 | 0.91 | [ |
| Mg-6Zn-0.2Ca-0.8Zr | 300°C, 0.12, 20:1 | 310 | 357 | 18 | 0.84 | |
| Mg-4.69Zn-0.48Ca | 250°C, -, 18:1 | 291 | 329 | 15.8 | - | [ |
| Mg-1.0Zn-0.2Ca | 350°C, 0.12, 16:1 | 120 | 200 | 40 | - | [ |
| Mg-1.0Zn-0.5Ca | 330°C, 0.12, 16:1 | 105 | 205 | 44 | - | |
| ZM61 | 350°C, 0.2-2.8, 25:1 | 209 | 305 | 11.5 | - | [ |
| ZM61 | 350°C, 0.2-2.8, 25:1, double aged | 338 | 366 | 5.2 | - | |
| Mg-6Zn-1Mn-4Sn | 350°C, 3, 25:1 | 250 | 330 | 11 | - | [ |
| Mg-6Zn-1Mn-4Sn | 350°C, 3, 25:1, double aged | 378 | 390 | 4.16 | - | |
| Mg-5.25Zn-0.6Ca | 300°C, 0.12, 20:1 | 220 | 265 | 21.4 | - | [ |
| Mg-5.25Zn-0.6Ca-0.3Mn | 300°C, 0.12, 20:1 | 272 | 303 | 18.9 | - | |
| Mg-6Zn-1Si-0.5Mn | 350°C, 0.48, 25:1 | 200 | 316 | 20.6 | - | [ |
| Mg-6Zn-1Si-0.5Mn | 350°C, 0.48, 25:1, T5 | 290 | 320 | 16 | - | |
| Mg-6Zn-1Si-0.5Mn-0.2Ca | 350°C, 0.48, 25:1, double aged | 330 | 360 | 12.5 | - | |
| Mg-0.21Zn-0.3Ca-0.14Mn | 300°C, 6, 20:1 | 100 | 185 | 32 | - | [ |
| 300°C, 60, 20:1 | ~70 | ~177 | ~28 | - | ||
| Mg-0.53Zn-0.24Ca-0.27Mn | 300°C, 6, 20:1 | 108 | 200 | 33 | - | |
| 300°C, 60, 20:1 | ~75 | ~190 | ~30 | - | ||
| Mg-0.71Zn-0.36Ca-0.07Mn | 300°C, 6, 20:1 | 108 | 220 | 37 | - | |
| 300°C, 24, 20:1 | 95 | 193 | 34 | - | ||
| Mg-0.21Zn-0.30Ca-0.14Mn | 300°C, 1.2, 20:1 | 310 | 310 | 22 | 0.54 | [ |
| 400°C, 1.2, 20:1 | 115 | 210 | 32 | 0.78 | ||
| Mg-5.99Zn-1.76Ca-0.35Mn | 300°C, 0.12, 20:1 | 289 | 303 | 16 | 0.89 | [ |
| Mg-3.0Zn-1.0Sn-0.3Mn-0.3Ca | 200°C, 60, 30:1 | 220 | 282 | 12 | - | [ |
| 300°C, 60, 30:1 | 187 | 301 | 19.6 | - | ||
| Mg-4Zn-2Al-2Sn | 225°C, 1-2, 61:1 | 211 | 317 | 27.6 | 0.88 | [ |
| 250°C, 1-2, 61:1 | 176 | 296 | 24 | 0.89 | ||
| 275°C, 1-2, 61:1 | 173 | 293 | 23.6 | 0.95 |
Table 2 Typical mechanical properties of selected Mg-Zn extrusion alloys [37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, 50, 51]
| Compositions (wt%) | Extrusion parameters T, v (m/min), r | YS (MPa) | UTS (MPa) | El (%) | YR | Ref. |
|---|---|---|---|---|---|---|
| Mg-1.0Zn | 350°C, 0.12, 16:1 | 148 | 230 | 16.2 | - | [ |
| Mg-2Zn | 320°C, -, 23.6:1 | 115 | 192 | 22.8 | - | [ |
| Mg-6Zn | 250°C, -, 8:1 | 169.5 | 279.5 | 18.8 | - | [ |
| Mg-6.2Zn (Z6) | 350°C, 0.12, 20:1. | 162 | 290 | 21 | - | [ |
| 350°C, 0.12, 20:1, T6 | 254 | 318 | 17.3 | - | ||
| Mg-6.2Zn-0.6Zr | 350°C, 0.12, 20:1. | 244 | 317 | 13.8 | - | |
| 350°C, 0.12, 20:1, T6 | 275 | 318 | 17.1 | - | ||
| Mg-6Zn-0.2Ca | 300°C, 0.12, 20:1 | 148 | 275 | 26 | 0.91 | [ |
| Mg-6Zn-0.2Ca-0.8Zr | 300°C, 0.12, 20:1 | 310 | 357 | 18 | 0.84 | |
| Mg-4.69Zn-0.48Ca | 250°C, -, 18:1 | 291 | 329 | 15.8 | - | [ |
| Mg-1.0Zn-0.2Ca | 350°C, 0.12, 16:1 | 120 | 200 | 40 | - | [ |
| Mg-1.0Zn-0.5Ca | 330°C, 0.12, 16:1 | 105 | 205 | 44 | - | |
| ZM61 | 350°C, 0.2-2.8, 25:1 | 209 | 305 | 11.5 | - | [ |
| ZM61 | 350°C, 0.2-2.8, 25:1, double aged | 338 | 366 | 5.2 | - | |
| Mg-6Zn-1Mn-4Sn | 350°C, 3, 25:1 | 250 | 330 | 11 | - | [ |
| Mg-6Zn-1Mn-4Sn | 350°C, 3, 25:1, double aged | 378 | 390 | 4.16 | - | |
| Mg-5.25Zn-0.6Ca | 300°C, 0.12, 20:1 | 220 | 265 | 21.4 | - | [ |
| Mg-5.25Zn-0.6Ca-0.3Mn | 300°C, 0.12, 20:1 | 272 | 303 | 18.9 | - | |
| Mg-6Zn-1Si-0.5Mn | 350°C, 0.48, 25:1 | 200 | 316 | 20.6 | - | [ |
| Mg-6Zn-1Si-0.5Mn | 350°C, 0.48, 25:1, T5 | 290 | 320 | 16 | - | |
| Mg-6Zn-1Si-0.5Mn-0.2Ca | 350°C, 0.48, 25:1, double aged | 330 | 360 | 12.5 | - | |
| Mg-0.21Zn-0.3Ca-0.14Mn | 300°C, 6, 20:1 | 100 | 185 | 32 | - | [ |
| 300°C, 60, 20:1 | ~70 | ~177 | ~28 | - | ||
| Mg-0.53Zn-0.24Ca-0.27Mn | 300°C, 6, 20:1 | 108 | 200 | 33 | - | |
| 300°C, 60, 20:1 | ~75 | ~190 | ~30 | - | ||
| Mg-0.71Zn-0.36Ca-0.07Mn | 300°C, 6, 20:1 | 108 | 220 | 37 | - | |
| 300°C, 24, 20:1 | 95 | 193 | 34 | - | ||
| Mg-0.21Zn-0.30Ca-0.14Mn | 300°C, 1.2, 20:1 | 310 | 310 | 22 | 0.54 | [ |
| 400°C, 1.2, 20:1 | 115 | 210 | 32 | 0.78 | ||
| Mg-5.99Zn-1.76Ca-0.35Mn | 300°C, 0.12, 20:1 | 289 | 303 | 16 | 0.89 | [ |
| Mg-3.0Zn-1.0Sn-0.3Mn-0.3Ca | 200°C, 60, 30:1 | 220 | 282 | 12 | - | [ |
| 300°C, 60, 30:1 | 187 | 301 | 19.6 | - | ||
| Mg-4Zn-2Al-2Sn | 225°C, 1-2, 61:1 | 211 | 317 | 27.6 | 0.88 | [ |
| 250°C, 1-2, 61:1 | 176 | 296 | 24 | 0.89 | ||
| 275°C, 1-2, 61:1 | 173 | 293 | 23.6 | 0.95 |
| Compositions (wt%) | Extrusion parameters T, v (m/min), r | YS (MPa) | UTS (MPa) | El (%) | YR | Ref. |
|---|---|---|---|---|---|---|
| Mg-1.05Ca-0.097Mn | 300°C, 2.4, 20:1 | 310 | - | 6.5 | - | [ |
| 350°C, 2.4, 20:1 | 280 | - | 11 | - | ||
| Mg-0.41Ca-0.4Al-0.02Mn | 350°C, 0.86-1.41, 19.6:1 | ~165 | ~234 | ~34 | - | [ |
| Mg-0.84Ca-0.4Al-0.02Mn | 350°C, 0.86-1.41, 19.6:1 | ~185 | ~239 | ~19.5 | - | |
| Mg-1.89Ca-0.4Al-0.02Mn | 350°C, 0.86-1.41, 19.6:1 | ~204 | ~252 | ~14.9 | - | |
| Mg-2.85Ca-0.4Al-0.02Mn | 350°C, 0.86-1.41, 19.6:1 | ~248 | ~273 | ~7.3 | - | |
| Mg-0.5Ca | 350°C, -, 4:1+236°C, -, 25:1 | 420 | - | ~7.5 | - | [ |
| Mg-1.0Ca-0.5Sr | 275°C, -, 25:1 | ~304 | ~307 | ~10.4 | ~0.82 | [ |
| 340°C, -, 25:1 | ~202 | ~234 | ~18.3 | ~0.90 | ||
| 400°C, -, 25:1 | ~157 | ~215 | ~18.7 | ~0.87 | ||
| Mg-1Ca-1Zn-0.6Zr | 350°C, 0.18, 30:1 | 306 | 314 | 10.3 | - | [ |
| 400°C, 0.18, 30:1 | 262 | 291 | 11.7 | - | ||
| Mg-2Sn-2Ca | 220°C, 0.36, 20:1 | 443 | 460 | 1.2 | 0.72 | [ |
| 240°C, 0.36, 20:1 | 420 | 435 | 3.0 | 0.73 | ||
| 280°C, 0.36, 20:1 | 386 | 414 | 5.8 | 0.90 | ||
| 320°C, 0.36, 20:1 | 358 | 365 | 8.9 | - |
Table 3 Typical mechanical properties of selected Mg-Ca extrusion alloys [55, 56, 57, 58, 59, 60]
| Compositions (wt%) | Extrusion parameters T, v (m/min), r | YS (MPa) | UTS (MPa) | El (%) | YR | Ref. |
|---|---|---|---|---|---|---|
| Mg-1.05Ca-0.097Mn | 300°C, 2.4, 20:1 | 310 | - | 6.5 | - | [ |
| 350°C, 2.4, 20:1 | 280 | - | 11 | - | ||
| Mg-0.41Ca-0.4Al-0.02Mn | 350°C, 0.86-1.41, 19.6:1 | ~165 | ~234 | ~34 | - | [ |
| Mg-0.84Ca-0.4Al-0.02Mn | 350°C, 0.86-1.41, 19.6:1 | ~185 | ~239 | ~19.5 | - | |
| Mg-1.89Ca-0.4Al-0.02Mn | 350°C, 0.86-1.41, 19.6:1 | ~204 | ~252 | ~14.9 | - | |
| Mg-2.85Ca-0.4Al-0.02Mn | 350°C, 0.86-1.41, 19.6:1 | ~248 | ~273 | ~7.3 | - | |
| Mg-0.5Ca | 350°C, -, 4:1+236°C, -, 25:1 | 420 | - | ~7.5 | - | [ |
| Mg-1.0Ca-0.5Sr | 275°C, -, 25:1 | ~304 | ~307 | ~10.4 | ~0.82 | [ |
| 340°C, -, 25:1 | ~202 | ~234 | ~18.3 | ~0.90 | ||
| 400°C, -, 25:1 | ~157 | ~215 | ~18.7 | ~0.87 | ||
| Mg-1Ca-1Zn-0.6Zr | 350°C, 0.18, 30:1 | 306 | 314 | 10.3 | - | [ |
| 400°C, 0.18, 30:1 | 262 | 291 | 11.7 | - | ||
| Mg-2Sn-2Ca | 220°C, 0.36, 20:1 | 443 | 460 | 1.2 | 0.72 | [ |
| 240°C, 0.36, 20:1 | 420 | 435 | 3.0 | 0.73 | ||
| 280°C, 0.36, 20:1 | 386 | 414 | 5.8 | 0.90 | ||
| 320°C, 0.36, 20:1 | 358 | 365 | 8.9 | - |
Fig. 2 a, b Optical micrographs. c, d TEM images of the as-extruded samples. a, c are the sample extruded at 300°C and b, d are the sample extruded at 350°C. The enlarged morphology of typical nanoparticles in c and the corresponding FFT patterns are included in c1 and c2. Textures of the extruded samples are also shown in e. Extrusion direction and radial direction are marked as ED and RD, respectively [55]
Fig. 3 Typical TEM images of as-extruded samples, a, b TX22-220, c, d TX22-240, e, f TX22-280 alloys. LAGBs are marked by yellow arrows, and the dislocations are marked by red arrows. Nanoprecipitates are circled by the blue ellipses [60]
| Compositions (wt%) | Extrusion parameters T, v (m/min), r | YS (MPa) | UTS (MPa) | El (%) | YR | Ref. |
|---|---|---|---|---|---|---|
| Mg-2Sn | 260°C, 2.4, 20:1. | 157 | 230 | 16 | - | [ |
| Mg-6Sn | 300°C, 25, 25:1. | 191 | 252 | 20.5 | - | [ |
| ATM150 | 300°C, 25, 25:1. | 248 | 294 | 20.6 | - | |
| ATM350 | 300°C, 25, 25:1. | 240 | 315 | 15.2 | - | |
| ATM650 | 300°C, 25, 25:1. | 232 | 346 | 15.6 | - | |
| ATM950 | 300°C, 25, 25:1. | 298 | 370 | 8.2 | - | |
| Mg-9.3Sn-2.45Zn-0.21Mn | 260°C, 2.8, 56:1. | 163 | 274 | 22 | - | [ |
| 260°C, 2.8, 56:1, T6. | 190 | 260 | 12 | - | ||
| Mg-9.8Sn-1.2Zn-1.0Al | 250°C, 0.12, 20:1. | 308 | 354 | 12 | 0.9 | [ |
| TAZ1031 | 250°C, 0.12, 20:1. | 319 | 358 | 6.1 | 1.00 | [ |
| 300°C, 2.4, 20:1. | 228 | 329 | 13.3 | 1.08 | ||
| 400°C, 2.4, 20:1. | 214 | 315 | 11.0 | 0.96 | ||
| TAZ1031-0.1Na | 300°C, 0.12, 20:1. | 336 | 362 | 3.1 | 0.94 | |
| TZAM5420 | 300°C, 0.12-2.4, 20:1. | 182 | 324 | 24 | - | [ |
| 300°C, 0.12-2.4, 20:1, T6 | 186 | 292 | 19 | - | ||
| TZAM5420-0.1Na | 300°C, 0.12-2.4, 20:1. | 243 | 324 | 10 | - | |
| 300°C, 0.12-2.4, 20:1, T6 | 347 | 369 | 3 | - | ||
| TZAM6620 | 300°C, 0.12-2.4, 20:1. | 247 | 349 | 16 | 1.02 | |
| 300°C, 0.12-2.4, 20:1, double aged | 370 | 399 | 14 | 0.83 | ||
| Mg-8Sn-2Zn-0.2Mn | 300°C, 0.48, 28:1 | 321.5 | 360.2 | 12.26 | - | [ |
| Mg-8Sn-2Zn-0.2Mn-0.5Cu | 300°C, 0.48, 28:1 | 365.9 | 388.4 | 5.8 | - | |
| TX21 | 260°C, 2.4, 20:1 | 269 | 305 | 6 | - | [ |
| TXZ212 | 260°C, 2.4, 20:1 | 218 | 285 | 23 | - | |
| Mg-8Sn-1Al-1Zn | 250°C, 2, 25:1 | 244 | 312 | 17.5 | - | [ |
| 250°C, 4.5, 25:1 | 231 | 311 | 15.2 | - | ||
| 250°C, 10, 25:1 | 199 | 286 | 14.8 | - | ||
| TAZ711 | 350°C, 9, 50:1 | 194 | 271 | 13.4 | - | [ |
| TAZ711 | 350°C, 19, 50:1 | 184 | 250 | 13.4 | - | |
| TAZ711 | 350°C, 27, 50:1 | 180 | 240 | 12.9 | - |
Table 4 Typical mechanical properties of selected Mg-Sn-based extrusion alloys [62, 63, 64, 65, 66, 67, 68, 69, 70]
| Compositions (wt%) | Extrusion parameters T, v (m/min), r | YS (MPa) | UTS (MPa) | El (%) | YR | Ref. |
|---|---|---|---|---|---|---|
| Mg-2Sn | 260°C, 2.4, 20:1. | 157 | 230 | 16 | - | [ |
| Mg-6Sn | 300°C, 25, 25:1. | 191 | 252 | 20.5 | - | [ |
| ATM150 | 300°C, 25, 25:1. | 248 | 294 | 20.6 | - | |
| ATM350 | 300°C, 25, 25:1. | 240 | 315 | 15.2 | - | |
| ATM650 | 300°C, 25, 25:1. | 232 | 346 | 15.6 | - | |
| ATM950 | 300°C, 25, 25:1. | 298 | 370 | 8.2 | - | |
| Mg-9.3Sn-2.45Zn-0.21Mn | 260°C, 2.8, 56:1. | 163 | 274 | 22 | - | [ |
| 260°C, 2.8, 56:1, T6. | 190 | 260 | 12 | - | ||
| Mg-9.8Sn-1.2Zn-1.0Al | 250°C, 0.12, 20:1. | 308 | 354 | 12 | 0.9 | [ |
| TAZ1031 | 250°C, 0.12, 20:1. | 319 | 358 | 6.1 | 1.00 | [ |
| 300°C, 2.4, 20:1. | 228 | 329 | 13.3 | 1.08 | ||
| 400°C, 2.4, 20:1. | 214 | 315 | 11.0 | 0.96 | ||
| TAZ1031-0.1Na | 300°C, 0.12, 20:1. | 336 | 362 | 3.1 | 0.94 | |
| TZAM5420 | 300°C, 0.12-2.4, 20:1. | 182 | 324 | 24 | - | [ |
| 300°C, 0.12-2.4, 20:1, T6 | 186 | 292 | 19 | - | ||
| TZAM5420-0.1Na | 300°C, 0.12-2.4, 20:1. | 243 | 324 | 10 | - | |
| 300°C, 0.12-2.4, 20:1, T6 | 347 | 369 | 3 | - | ||
| TZAM6620 | 300°C, 0.12-2.4, 20:1. | 247 | 349 | 16 | 1.02 | |
| 300°C, 0.12-2.4, 20:1, double aged | 370 | 399 | 14 | 0.83 | ||
| Mg-8Sn-2Zn-0.2Mn | 300°C, 0.48, 28:1 | 321.5 | 360.2 | 12.26 | - | [ |
| Mg-8Sn-2Zn-0.2Mn-0.5Cu | 300°C, 0.48, 28:1 | 365.9 | 388.4 | 5.8 | - | |
| TX21 | 260°C, 2.4, 20:1 | 269 | 305 | 6 | - | [ |
| TXZ212 | 260°C, 2.4, 20:1 | 218 | 285 | 23 | - | |
| Mg-8Sn-1Al-1Zn | 250°C, 2, 25:1 | 244 | 312 | 17.5 | - | [ |
| 250°C, 4.5, 25:1 | 231 | 311 | 15.2 | - | ||
| 250°C, 10, 25:1 | 199 | 286 | 14.8 | - | ||
| TAZ711 | 350°C, 9, 50:1 | 194 | 271 | 13.4 | - | [ |
| TAZ711 | 350°C, 19, 50:1 | 184 | 250 | 13.4 | - | |
| TAZ711 | 350°C, 27, 50:1 | 180 | 240 | 12.9 | - |
| Compositions (wt%) | Extrusion parameters T, v (m/min), r | YS (MPa) | UTS (MPa) | EL (%) | YR | Ref. |
|---|---|---|---|---|---|---|
| Mg | 300°C, 0.06, 36:1. | 120 | 208 | 12 | 0.74 | [ |
| Mg-6Bi | 300°C, 0.06, 36:1. | 189 | 228 | 19 | 1.01 | [ |
| BAZ811 | 300°C, 1.98, 30:1. | 291 | 331 | 14.6 | 0.94 | [ |
| AZ31 | 300°C, 1.98, 30:1. | 200 | 284 | 24.5 | 0.84 | [ |
| Mg-5Bi-1Si | RS, -, -, 19.1:1. | - | 240 | 40 | - | [ |
| Mg-5Bi-1Ca | RS, -, -, 19.1:1. | - | 205 | 45 | - | [ |
| Mg-2.5Bi | 110°C, -, -. | - | 155 | 170 | - | [ |
Table 5 Typical mechanical properties of selected Mg-Bi extrusion alloys [72, 73, 74, 75]
| Compositions (wt%) | Extrusion parameters T, v (m/min), r | YS (MPa) | UTS (MPa) | EL (%) | YR | Ref. |
|---|---|---|---|---|---|---|
| Mg | 300°C, 0.06, 36:1. | 120 | 208 | 12 | 0.74 | [ |
| Mg-6Bi | 300°C, 0.06, 36:1. | 189 | 228 | 19 | 1.01 | [ |
| BAZ811 | 300°C, 1.98, 30:1. | 291 | 331 | 14.6 | 0.94 | [ |
| AZ31 | 300°C, 1.98, 30:1. | 200 | 284 | 24.5 | 0.84 | [ |
| Mg-5Bi-1Si | RS, -, -, 19.1:1. | - | 240 | 40 | - | [ |
| Mg-5Bi-1Ca | RS, -, -, 19.1:1. | - | 205 | 45 | - | [ |
| Mg-2.5Bi | 110°C, -, -. | - | 155 | 170 | - | [ |
| Process | Schematic illustration | Equivalent strain | Ref. |
|---|---|---|---|
| (a) Equal channel angular pressing (ECAP) | | ?=N 2×3-1/2 cotφ, N, the number of ECAP passes | [ |
| (b) Extrusion shear (ES) | | - | [ |
| (c) Cyclic extrusion compression (CEC) | | ?=N 4ln(D/d) N, number of cycles | [ |
| (d) Repetitive upsetting extrusion (RUE) | | ?=3/2 ln(d0/d1)+2ln(d1/d0) d1, the chamber diameter, d0, the channel diameter | [ |
| (e) Accumulative back extrusion (ABE) | | - | [ |
Table 6 Schematic illustration of some basic and modern SPD techniques [111, 112, 113, 114, 115, 116]
| Process | Schematic illustration | Equivalent strain | Ref. |
|---|---|---|---|
| (a) Equal channel angular pressing (ECAP) | | ?=N 2×3-1/2 cotφ, N, the number of ECAP passes | [ |
| (b) Extrusion shear (ES) | | - | [ |
| (c) Cyclic extrusion compression (CEC) | | ?=N 4ln(D/d) N, number of cycles | [ |
| (d) Repetitive upsetting extrusion (RUE) | | ?=3/2 ln(d0/d1)+2ln(d1/d0) d1, the chamber diameter, d0, the channel diameter | [ |
| (e) Accumulative back extrusion (ABE) | | - | [ |
|
| [1] | X.L. Wang, J.Y. Li, Q.S. Mei. Recent progress in Zn matrix composites for biomedical applications [J]. Metals Advances, 2026, 39(1): 26-37. |
| [2] | Yuanyuan Feng, Jianchao Pang, Xiaoyuan Teng, Chenglu Zou, Jingjing Liang, Yuping Zhu, Shouxin Li, Jinguo Li, Zhefeng Zhang. Quasi-in-situ EBSD Study on the Microstructure and Tensile Properties of Selective Laser Melted Inconel 718 Alloy Processed by Different Heat Treatments [J]. Acta Metallurgica Sinica (English Letters), 2025, 38(9): 1499-1512. |
| [3] | F. S. Li, L. H. Wu, Y. Kan, H. B. Zhao, D. R. Ni, P. Xue, B. L. Xiao, Z. Y. Ma. Microstructure Evolution and Fracture Mechanisms in Electron Beam Welded Joint of Ti-6Al-4V ELI Alloy Ultra-thick Plates [J]. Acta Metallurgica Sinica (English Letters), 2025, 38(8): 1317-1330. |
| [4] | Haoyu Cheng, Chenyang Hou, Jianlei Zhang, Xiaodong Mao, Yuanxiang Zhang, Yanyun Zhao, Chulun Shen, Changjiang Song. An Innovative Large-Scale Preparation Method for ODS Steel: Zone Melting with Built-In Precursor Powder [J]. Acta Metallurgica Sinica (English Letters), 2025, 38(8): 1397-1409. |
| [5] | Haoran Pang, Liwei Lu, Gongji Yang, Xiaojun Wang, Wen Wang, Hua Zhang, Yujuan Wu. Amelioration of Mechanical Properties of Rolled Mg-4.5Al-2.5Zn Alloy by Cryogenic Cycling Treatment [J]. Acta Metallurgica Sinica (English Letters), 2025, 38(8): 1436-1452. |
| [6] | Qi Zhou, Yufeng Xia, Yu Duan, Baihao Zhang, Yuqiu Ye, Peitao Guo, Lu Li. Microstructure and Mechanical Properties of Yb-Containing AZ80 Cast Alloys [J]. Acta Metallurgica Sinica (English Letters), 2025, 38(7): 1095-1108. |
| [7] | Yuanxiao Dai, Yue Zhang, Mei Wang, Jie Liu, Yaobo Hu, Bin Jiang. Three-Point Bending Deformation Behavior of a High Plasticity Mg-2.6Er-0.6Zr Alloy Sheet [J]. Acta Metallurgica Sinica (English Letters), 2025, 38(7): 1109-1126. |
| [8] | Mengjun Chen, Tingping Hou, Shi Cheng, Feng Hu, Tao Yu, Xianming Pan, Yuanyuan Li, Kaiming Wu. A Comprehensive Exploration of the Relationship between Microstructure Optimization and Strength Enhancement in Low-Density 5Al-5Mn Steel [J]. Acta Metallurgica Sinica (English Letters), 2025, 38(7): 1219-1236. |
| [9] | Wei Pan, Bin Xu, Chong Li. Effects of Groove Shape on Microstructure and Mechanical Responses of Laser-Directed Energy Deposition-Repaired GH4099 Ni-Based Superalloy [J]. Acta Metallurgica Sinica (English Letters), 2025, 38(6): 1003-1011. |
| [10] | Xiang Fei, Naicheng Sheng, Zhaokuang Chu, Han Wang, Shijie Sun, Yuping Zhu, Shigang Fan, Jinjiang Yu, Guichen Hou, Jinguo Li, Yizhou Zhou, Xiaofeng Sun. Design Strategy for Synergistic Strengthening of W and Al in High-W Superalloys [J]. Acta Metallurgica Sinica (English Letters), 2025, 38(6): 1057-1068. |
| [11] | Yao Zhang, Hongtao Wang, Zhongtao Lu, Zifeng Li, Pengfei Wen, Xiaobin Feng, Guodong Li, Bo Duan, Pengcheng Zhai. Effect of Ag Vacancies on the Mechanical Properties of Ag2S Thermoelectric Semiconductor [J]. Acta Metallurgica Sinica (English Letters), 2025, 38(5): 869-875. |
| [12] | Yaoxiang Geng, Keying Lv, Chunfeng Zai, Zhijie Zhang, Anil Kunwar. A High-Strength TiB2-Modified Al-Si-Mg-Zr Alloy Fabricated by Laser Powder-Bed Fusion [J]. Acta Metallurgica Sinica (English Letters), 2025, 38(4): 542-554. |
| [13] | Haijian Liu, Tianle Li, Xifeng Li, Huiping Wu, Zhiqiang Wang, Jun Chen. Strength Optimization of Diffusion-Bonded Ti2AlNb Alloy by Post-Heat Treatment [J]. Acta Metallurgica Sinica (English Letters), 2025, 38(4): 614-626. |
| [14] | X. W. Shang, Z. G. Lu, R. P. Guo, L. Xu. Influence of Hot Isostatic Pressing Temperature on Microstructure and Mechanical Properties of Ti-6.5Al-3.5Mo-1.5Zr-0.3Si Alloy [J]. Acta Metallurgica Sinica (English Letters), 2025, 38(4): 627-641. |
| [15] | Jing Wang, Xuejian Wang, Zongning Chen, Huijun Kang, Tongmin Wang, Enyu Guo. In Vitro Corrosion Behavior and Mechanical Property of Novel Mg-Sn-In-Ga Alloys for Orthopedic Applications [J]. Acta Metallurgica Sinica (English Letters), 2025, 38(3): 353-366. |
| Viewed | ||||||
|
Full text |
|
|||||
|
Abstract |
|
|||||
WeChat